Prefabrizéiert Streck
Produit Typ
|
Methoden | Unitéiten | Konditiounen | Resultater | Ufuerderunge | Pass/Ausgefall |
Tensile Eegeschafte
|
EN 12230
|
Mpa
|
Nei, 23 ° C | 0,54 | > 0,40 eng
|
Pass |
No A/W Aging (1) | 0,55 | Pass | ||||
Nom Spike Resistance ⑵ | 0,50 | Pass | ||||
No A/W Aging (1) + Spike Resistenz (2) | 0.49 | Pass | ||||
Variatioun (%)
|
Nom Spike Resistance ⑵ | 7 | <20
|
Pass | ||
No A/W Aging (1) +
Spike Resistenz ⑵ |
11 | Pass | ||||
Verlängerung an der Paus
|
EN 12230
|
%
|
Nei, 23 ° C | 61 | > 40
|
Pass |
Nom Aging ⑴ | 52 | Pass | ||||
Nom Spike Resistance ⑵ | 70 | Pass | ||||
Nom A/W Aging ⑴ + Spike Resistance ⑵ | 42 | Pass | ||||
Variatioun (%)
|
Nom Spike Resistance ⑵ | 15 | <20
|
Pass | ||
No A/W Aging (1) + Spike Resistenz ⑵ | 19 | Pass | ||||
Resistenz géint Verschleiung | EN ISO 5470-1 | g | Nei, 23 ° C | 2.8 | <4.0 vum Masseverloscht tëscht 500 an 1500 Zyklen | Pass |
Waasser permeabilitéit | EN 12616 | mm/h | Nei, 23 ° C | > 2000 ewechzekréien | > 150 mm/h | Pass |
Absolut Déck | EN 1969 (Method A) | mm | Nei, 23 ° C | 13.0 | > 10 | Pass |
Allgemeng Déck | EN 1969 (Method A) | mm | Nei, 23 ° C | 13.6 | - | - |
Dimensiounen
(1) A/ W Aging - Waarm Loftalterung + waarmt Waasseralterung
D'waarm Loft a Waasseralterung gëtt nom EN 13817 Standard ausgefouert an direkt nom EN 13744 Standard. No der Uewerflächbeliichtung ginn déi folgend Eegeschafte erëm gemooss fir eng potenziell Ännerung ze kontrolléieren:
Schockabsorptioun
Zucheigenschaften / Verlängerung bei der Paus
(2) Spike Resistenz
De Spike Resistenz Test gëtt no Testmethod ausgefouert, beschriwwen am EN 14810 Standard.